CERAMIC COATING APPLICATION
1 - Sandblast with aluminum
oxide. DO NOT USE glass bead or sand.
2 - Degrease with acetone, lacquer
thinner, M.E.K . or similar non petroleum
based material
3 - Spray with an airbrush or
detail touch up gun or similar equipment,
with fine spray pattern. Water based coatings
spray at 50 to 60 psi; solvent based coatings
spray at 35 to 40 psi.
Proper thickness is normally
achieved with one wet, solid colored coat
For coatings that require oven curing, most
coatings cure between 300f to 500f.
For
retail packaged products, requiring baking,
a standard kitchen oven or toaster oven may
be used.
COATINGS OR SOLVENTS SHOULD
NOT BE CURED IN ANY OVEN COMING IN CONTACT
WITH FOOD.
Ceramic coatings can be sanded
with 600 grit then 1500 grit wet dray paper
then polished with a buffer.